DN400 PN160 A105  全焊接球阀 20260709 (9) 拷贝

The test that happened before the weld

Every ball valve leaves the factory having been proved twice: a shell test at one and a half times its rating, and a seat test at one and one tenth. Both are done in a shop, at shop temperature, on a valve that is bolted to a test bench and connected to nothing that will ever be hot. Then the valve is packed, shipped, lifted onto a spool, aligned, and welded. From that moment, everything the certificate says about the seat is a statement about a different valve.

This is not a story about a bad valve, and it is not a workmanship story. It is a story about the one event in a valve's life that the factory test cannot anticipate. A weld puts a temperature into the body that no part of the valve was designed to see, and the part that suffers is not the steel. It is the seat, and the small polymer parts around it, which are the only components in a ball valve with a ceiling measured on the same scale as a kitchen oven rather than a furnace.

The failure that results is quiet, late, and easy to blame on the wrong party. Nothing cracks. Nothing is scratched. The valve passed its shell test, passed the first week at pressure, and then began to weep — and by the time anyone opens it, the evidence of what happened has already been smoothed away by the very act of sealing.

Two temperatures that have nothing to do with each other

The weld pool is liquid steel. The seat is a polymer, an elastomer, or a composite of the two, chosen precisely because it is soft enough to conform to a lapped ball and elastic enough to keep conforming after a thousand cycles. Its useful range ends where the material stops behaving elastically, and that limit is a property of the material — published in every seat guide, and a small fraction of the temperature at which steel is welded, and a smaller fraction still of the temperature at which steel is stress relieved.

Put those two numbers in the same body and the outcome is not a matter of skill. The only variables the welder controls are how hot the seat gets and how long it stays there, and both are set by the wall thickness, the joint design and the qualified procedure rather than by intent. A careful welder on a small socket joint can keep the seat under its ceiling. The same welder, on a large girth weld with a preheat and a slow cool, cannot — the heat is in the procedure before he strikes an arc.

This is why ball valve welding heat is not a single event but a curve with a long tail. The arc lasts seconds; the body stays warm for hours; and the seat sits inside the part of the body that cools last.

How the heat actually arrives

There are three paths, and they do not arrive together. The first is conduction through the body wall. The arc heats the end of the body, and the metal carries that heat inward along the same wall that surrounds the seat pocket. This is the fast path, and it is fast for two reasons: steel conducts well, and the wall is thick. A thick wall holds more heat and gives it up for longer, which is why large valves are worse than small ones even though the seat is further from the arc. Distance buys a delay, not an exemption, because the section that has to be crossed is also the section that stores the most heat.

The second path is the cavity. A closed valve is a closed box. Whatever is inside it — air, or the product left over from the factory test, or the water from the shell test that was never fully drained — heats by radiation from the hot wall and by convection from the hot surfaces, and it has nowhere to go. A trapped gas in a closed cavity will reach a temperature that the outside of the body never shows, and it will hold that temperature while the outside is already cool enough to touch. A trapped liquid does something worse: it expands, and it loads the seats from behind while they are soft.

The third path is the geometry of the seat pocket, which is a cup surrounded by metal on three sides. Heat arrives through the pocket floor, through the bore side, and through the end face. There is no free surface for it to leave from, and no air gap to break the path. The seat occupies the one place in the valve where heat comes in from every direction and can only leave through the same metal that is still being heated.

This is also why the hand test is worthless as a check. The outside of a body can be cool enough to hold a palm while the pocket behind it is still far above the seat's ceiling, because the outside is radiating into air and the pocket is not. Coating is a better record than a hand: if the paint around the weld is discoloured, blistered or burnt, the seat has seen at least that temperature and probably more, and the discolouration is the only written evidence the valve will ever produce.

What heat does to a polymer seat

Nothing breaks, and that is exactly the problem. A seat that has been overheated looks, on a bench, like a seat that has simply been in service: the face is smooth, the contact band is even and often wider than expected, and there is no scratch, no gouge and no embedded particle to explain why the valve will not hold.

What has changed is the modulus. A polymer seat is held against the ball by a spring and, once the line is pressurised, by the medium behind it. The spring is chosen for the material's stiffness at working temperature, and the arithmetic only works if the material is still in its elastic range. Heat the seat and the stiffness falls away; the same load that produced an elastic squeeze now produces flow. The seat creeps into its pocket, the contact band widens and flattens, and the pressure per unit of contact area falls. When the valve cools, the seat does not come back to its old thickness. It has taken a set, and the interference that made the seal is now a gap.

The second casualty is the seal behind the seat — the O ring or lip seal that closes the joint between the seat ring and the body. Elastomers held under compression at temperature take a compression set too, and a seal that has taken a set stops following the small movements the seat makes on every cycle. The seat face can be perfect and the valve will still leak, because the leak is behind the seat rather than across it. This is the leak that gets misdiagnosed as a scored seat, replaced, and reproduced.

The third group is thinner and easier to forget: the dry film lubricant or polymer topcoat on the ball, the back up ring that stops the seat extruding, and, on a two piece body, the body gasket if the closure weld is close enough. All of them are polymers. All of them share the same ceiling. The packing is usually the one soft part that survives, not because it is protected by design but because it sits at the far end of the stem behind a long neck of metal, which is the only reason a stem seal outlives a seat during welding.

Why the leak appears weeks later

The sequence explains the timing, and the timing is what makes the diagnosis so hard. The factory seat test passed before the weld. The field shell test at one and a half times the rating is a shell test: it proves the body, the closure and the joints, and on a valve tested with the ball open it does not load the seat at all. The first time the seat is asked to seal after the weld is at commissioning — and by then the damage is done, invisible, and already several weeks old.

The leak then has a signature that sends people looking in the wrong place. A seat that has lost preload can hold at high differential pressure and weep at low pressure, because at pressure the medium itself pushes the seat into the ball, and at low pressure only the spring is left — the same spring that was sized for a seat with its original thickness. So the valve passes the hydrotest, passes the first week at full pressure, and weeps when the line is drained, when the pump stops, when the batch is finished. It is written up as an intermittent ball valve seat leak, the seat is replaced, and the replacement does exactly the same thing, because the cause was never the seat material.

The first thermal cycle completes the damage. Start up takes the valve to its working temperature and the ball, the seat and the body expand by different amounts. A seat that was marginal at ambient loses the last of its squeeze, and a weep becomes a drip. If the line is then cycled — a batch process, a day and night cycle, a seasonal shutdown — the seat is worked against a ball it no longer presses on, and the contact band starts to pick up the polished sheen that everyone afterwards reads as wear.

This is the ordinary shape of ball valve seat damage after a weld: a wide, even, polished band with no scratch, a seat that is measurably thinner than the drawing, and a leak that appears at low pressure rather than high.

The sign you can read on site, for nothing

There is a symptom that costs nothing to check and is almost never recorded: the valve turns easier than it did. Seat friction is a large part of the torque on a small valve, and a seat that has lost its squeeze has less of it. Operators notice, and say nothing, because a valve that turns easily is not a fault under any procedure. It is the earliest physical evidence that the seat has taken a set, and it usually precedes the first complaint by weeks.

The second sign is the seat test itself, done properly rather than as a formality: one and one tenth times the rating, in both directions, for the full duration, with the body cavity vented so that a leak past the seat cannot hide behind a pressurised cavity. A valve that holds from one side and weeps from the other has a seat that is no longer sitting square to the ball, which is precisely what a set looks like from the outside.

Stress relief is not a spike, it is a soak

Welding is short and violent. Post weld heat treatment is the opposite: the whole region is brought up to temperature and held there for hours so that residual stress can relax. For the steel this is a kindness. For the seat it is the worst case there is, because there is no cold end left to hide in. Every part of the body, including the pocket, arrives at the soak temperature and stays there for the duration, and the seat is not cooled by anything.

And it is not optional. Piping codes require stress relief for certain materials and wall thicknesses. Sour service specifications require it so that the weld and the heat affected zone stay under a hardness ceiling, and that ceiling is met by the procedure, not by inspection afterwards. A cast body with weld repairs is normally stress relieved before it is even machined. So the requirement is set by the pipe, the joint and the service — never by the valve — while the seat material is set by the process. Two decisions, made by two different people, written on two different lines of the same datasheet, and they can contradict each other with nobody noticing until a seat weeps in a plant that is already running. That is why the ball valve stress relief question is a materials question before it is a welding question.

That contradiction is the real subject here. It cannot be solved at the arc by a careful welder, and it cannot be solved afterwards by tightening anything. It is solved at the order, by choosing a valve whose seat survives the heat, or a connection that keeps the heat away from the seat, or a sequence in which the seat is simply not fitted when the heat arrives.

Four ways out, and what each one costs

Flange it instead. The weld moves onto a pipe end that is not part of the valve, and the valve is bolted in afterwards. Nothing about the seat changes, and the heat never enters the body. The cost is two gasketed joints where there would have been one weld, plus bolting, plus the clearance to swing a wrench — and a flange pair that has to agree on facing, bolt circle and standard, which is a separate conversation every time.

Order a metal seated ball valve. The seat's ceiling becomes the body's ceiling, so welding and stress relief stop being a threat to the sealing element. The cost is real and should be quoted honestly: a metal seat seals on a much narrower band, needs hard facing and careful lapping, needs more torque from the operator or the actuator, and forgives debris far less than a polymer seat does. It is the right answer for high temperature and for anything that will be stress relieved; it is the wrong answer for a dirty line that was specified soft for good reasons.

Push the weld away. Extended weld ends, or a pup piece welded onto the valve in the workshop, put distance between the arc and the seat. This is the most common answer and the weakest one, because distance only buys time. On a large girth weld the heat input is set by the wall and the procedure, and the heat front travels far enough that a seat well away from the arc is still at risk. The pup must also survive the valve's own shell test without yielding, which is a check that is routinely skipped when the pup is supplied by someone else.

Fit the seats afterwards. A two piece, three piece or top entry body can be welded with the internals out, stress relieved, tested, and only then assembled. The factory already does exactly this on fully welded bodies, and the order is worth copying: the body is welded closed, stress relieved, the caps dressed, the shell tested while the body is still empty, and only then do the ball, the seats and the stem go in. The field version of the same idea is to weld the valve as a spool with a dummy in place of the centre section, as the three piece weld end design allows, so that the seats and the body gasket never see the heat.

微信图片_2026-11-20_153322_155

The four answers are not ranked, and a project will often use two of them at once: a metal seated valve on a stress relieved line with extended ends, or a flanged soft seated valve where the piping is welded and the valve is not. What matters is that the choice is made before the order rather than discovered at commissioning.

What the order has to say

None of this can be decided by the supplier alone, because the supplier does not know how the valve will be joined. Five lines on the order remove the ambiguity before it becomes a claim.

State the joining method, and if it is a weld, state the heat treatment the joint will receive — not the procedure number, just whether the joint will be stress relieved and whether the line is in sour service. State the seat material and whether it has to survive that heat treatment, or state plainly that the seats will be fitted after it. State the post weld seat test: one and one tenth times the rating, both directions, full duration, cavity vented. State who owns the weld procedure and the hardness check, because both belong to the fabricator and neither can be verified by the valve maker once the arc has struck. And state the paperwork that has to travel with the valve: the material certificates to EN 10204 3.1 and, if the body itself was stress relieved, the heat treatment record.

That last line is the first thing cut when a project is late, and it is the only thing that answers the question six months later, when a seat is weeping and nobody can say whether the valve or the weld is responsible. A seat fitted after welding, with a chart, closes the argument before it starts.

What this is not

It is not an argument against a weld end ball valve. A weld removes a gasketed joint, and a gasketed joint is the most common leak path on any valve; for buried lines, sour service and high pressure the weld is the correct connection and the flange is the compromise. What matters is the order of operations: heat first, seats last, test after. A valve that is welded with its seats in place and then stress relieved has been through a process that no specification anticipated, and no amount of care at the arc will undo it afterwards.

The same logic applies to repair welds years later. A body repair on a valve that is already in service, with seats fitted, is a smaller version of the same problem with a worse outcome, because the valve is now surrounded by product and cannot be purged. If a body needs welding, the seats should come out first — which is one more reason to know, before the valve is installed, whether the body can be opened in place at all.

J-VALVES builds floating ball valves from 1/2 inch to 8 inch and trunnion mounted ball valves from 2 inch to 56 inch, DN15 to DN1400, in ASME Class 150 to 2500, with soft seats where the process allows and metal seats where the heat does not, with butt weld ends to ASME B16.25, with extended weld ends and pup pieces, and with bodies — two piece, three piece, top entry and fully welded — in which the internals can go in after the last heat. Shell tests run at one and a half times the rating and seat tests at one and one tenth, with certificates to EN 10204 3.1.

Frequently Asked Questions

Can a soft seated ball valve be welded into a line? Yes, and it is done every day, but the heat has to be managed rather than assumed away. Weld with the valve fully open, keep the arc as far from the seat pocket as the end design allows, use a procedure with the lowest heat input that still meets the code, and accept that on a large girth weld or a stress relieved joint the seat is at risk no matter how careful the welder is. If the joint will be stress relieved, the soft seat should not be in the valve when it happens.

Does post weld heat treatment damage a ball valve seat? It usually destroys it. Stress relief holds the whole region at a temperature for hours, well above the ceiling of any polymer seat, and there is no part of the body that stays cool enough to protect it. A valve that is stress relieved with its seats fitted will normally pass a shell test and fail a seat test, and the seat will look undamaged when it is removed.

Why does my ball valve leak after installation when it passed the factory test? Because the factory test happened before the weld. The field shell test proves the body and the joints, not the seat, and the first real seat test is at commissioning. A seat that has taken a set from welding heat typically holds at high differential pressure and weeps at low pressure, which is why the leak is reported as intermittent and why replacing the seat does not fix it.

How far from the weld is the seat safe? There is no universal distance, and any number quoted as a safe clearance should be treated with suspicion. Distance buys time rather than immunity, because a heavy section stores heat and releases it slowly, and the cavity carries heat to the seat by a path that has nothing to do with line of sight. Extended weld ends help; they do not make the question go away.

What is the difference between welding with the valve open and fitting the seats afterwards? Welding with the valve open protects the bore from spatter and keeps a closed ball from being distorted, but the seats are still in the body and still get hot. Fitting the seats afterwards removes the seats from the heat entirely, which is the only answer that works when the joint must be stress relieved. It requires a body that can be opened — two piece, three piece or top entry — or a workshop sequence in which the valve is welded as a spool around a dummy.

Related Products

Explore the Valves in This Article
Nominal Size: 1 inch / DN25, range 1/4 to 12 inch Pressure Class: ASME Class 150, 19.6 bar at 38°C; Class 300 optional Body Material: ASTM B148 C95800 nickel aluminum bronze Body Type: Two piece, bolted Ball: C95800, SS316 hard faced optional Stem: C95800 or SS316, blowout proof Seat: PTFE, RPTFE, PPL, or reinforced PTFE Packing: PTFE or graphite combined packing End Connection: Threaded NPT / BSPT, flanged RF to ASME B16.5 optional Service Temperature: -29°C to +150°C standard, +200°C high temperature version Seawater Velocity Limit: About 6 m/s clean, 4.5 m/s with sand Design Standard: API 608, ASME B16.34 Test Standard: API 598, ISO 5208 Operation: Lever standard, pneumatic or electric optional
Size Range: 2 to 56 inch (DN50 to DN1400) Pressure Class: ASME Class 150 to 2500 / PN20 to PN420 Body Material: WCB, LCB, CF8, CF8M, CF3M, duplex, alloy steel Ball: Stainless with hard chrome, ENP, Stellite or tungsten carbide overlay Seat: PTFE, RPTFE, PPL, or metal Stellite faced Seat Arrangement: SPE, DPE (DIB-1), or combination (DIB-2) Packing: Live loaded graphite, ISO 15848-1 qualified Fire Test: API 607, also API 6FA and ISO 10497 Fugitive Emission: ISO 15848-1 class B or A, with temperature and cycle class stated Face to Face: ASME B16.10 short or long pattern End Connection: Flanged RF / RTJ to B16.5 and B16.47, butt weld to B16.25 Features: Double block and bleed, sealant injection, anti-static, anti-blowout stem Design Standard: API 6D, API 608, ASME B16.34, ISO 14313 Operation: Lever, gear, pneumatic, electric, hydraulic, gas over oil Sour Service: NACE MR0175 available
Nominal Size: 1-1/2 inch / DN40 Pressure Rating: 1000 WOG (68.9 bar cold working, non-shock) Body Type: Three piece, bolted end caps, four body bolts Body Material: ASTM A351 CF8 (304), CF8M (316) optional Ball: CF8, polished Ra 0.4 µm, full or reduced bore Seat: PTFE, RPTFE, PPL, or Stellite faced metal Body Gasket: PTFE to 180°C, graphite above Packing: PTFE V-ring to 200°C, graphite above End Connection: NPT, BSP, socket weld B16.11, butt weld B16.25, flanged RF Actuator Mounting: ISO 5211 F05 / F07 pad Air Supply: 0.4 to 0.7 MPa clean dry air Service Temperature: -29°C to +260°C, seat dependent Design Reference: MSS SP-110 general purpose, ASME B16.34 body wall Test Standard: API 598, ISO 5208
Nominal Size: 3/4 x 1/2 inch (DN20 x DN15), reduced bore Pressure Class: ASME Class 600 / PN100, 102.1 bar at 38°C Body Material: ASTM A182 F51 forged duplex, UNS S31803 PREN: Approximately 35 Ball: F51 with HVOF tungsten carbide or Stellite overlay Stem: F51, SS316 or 17-4PH, blowout proof Seat: RPTFE, Devlon, PEEK, or Stellite faced metal Bolting: B8M Class 2, alloy 718, or B7M for sour service End Connection: NPT, BSP, socket weld ASME B16.11, butt weld ASME B16.25 Bleed Port: Cavity bleed with plug or needle valve, lockable option Service Temperature: -29°C to +300°C, seat dependent Design Standard: API 6D, API 608, ASME B16.34 Test Standard: API 598, ISO 5208, cavity test through bleed port Sour Service: NACE MR0175 available