J-VALVES · Ball Valve Manufacturer · Wenzhou, China info@j-valves.com +86-13600648865

API 6D ball valve selection guide

News

Home News Bayer Process Ball Valves: A Valve That Machines Its Own Seat Groove
Inquire
Tungsten carbide coated ball and seat in a DN200 class 300 metal seated ball valve for Bayer process red mud blowdown

A DN200 metal seated ball valve came off the blowdown line between a digester and the first flash tank after nine weeks in service. The body was sound. The bore was sound. The ball had a groove in it four millimetres deep and six millimetres wide, running right around the ball on the circle where the seat had been touching it, with edges sharp enough to catch a fingernail. The seat ring carried a matching step worn into its face. Everything in that valve that had not been in the narrow gap between ball and seat, including parts that had sat in the same liquor at the same temperature for the same nine weeks, was close to new.

The maintenance report called it erosion and asked for a harder ball. That is the natural reading and it is wrong in a way that costs a refinery a set of trim every two months for years, because a harder ball will also groove, only later. Almost nothing flowed across that ball. The valve was shut. What flowed was the small quantity of liquor that got past the seat, and it flowed through a gap measured in tenths of a millimetre at a velocity no pipe in the plant ever sees. The valve was not eroded by the process. It was machined by its own seat clearance, with the process acting as the cutting compound.

What follows is the arithmetic: what the digestion train actually contains, why isolation and letdown cannot share one body, how thirty bar of pressure becomes ninety volumes of flash, why the groove deepens itself once it exists, which of the six minerals in red mud does the cutting, and why the caustic that everyone blames is actually a cracking problem rather than a corrosion problem. It ends with six clauses that would have doubled the life of that valve, none of which is a material grade.

1. What a digestion train asks of a valve

A Bayer refinery is a caustic loop with a solids problem bolted to the front of it. Bauxite arrives with 45 to 60 percent alumina of which 30 to 40 points are extractable, 5 to 30 percent iron oxide, 1 to 10 percent silica and, in the ores that decide valve life, 0.5 to 3 percent quartz. It is ground to a median of 50 to 150 micrometres and mixed with spent liquor carrying 150 to 260 grams per litre of sodium hydroxide expressed as sodium oxide, at a solids loading of 30 to 40 percent by weight. The mixture is then held at temperature long enough for the alumina to dissolve, and the whole point of the exercise is that everything else does not.

The temperature is not a process choice so much as a property of the ore. Gibbsite dissolves readily and needs 140 to 150 degrees C, which is 4 to 6 bar of saturated steam. Boehmite needs 200 to 240 degrees C. Diaspore, which is what a refinery in China or Greece is usually built around, needs 240 to 280 degrees C at 30 to 45 bar. That single sentence explains why two refineries with identical flow sheets run valve populations that fail in completely different ways.

Stage

What is in the pipe

Conditions

What the valve has to survive

Ground bauxite feed

dry ore, 50 to 150 micrometre

ambient, 1 to 3 bar

Attrition of the seat face by dry angular particles; no liquid to cushion anything

Pre-desilication

slurry at 30 to 35 percent solids

100 to 110 degrees C, 3 to 6 bar

Slow abrasion and heavy scaling, at velocities low enough that geometry wins

Digestion, gibbsite ore

slurry, 200 g/L Na2O

145 degrees C, 5 bar

Caustic cracking of the body, and scale on every hot surface

Digestion, diaspore ore

slurry, 240 to 260 g/L Na2O

240 to 260 degrees C, 32 to 45 bar

The same two, plus a thermal expansion problem across every flange

Blowdown to flash

the same slurry, flashing

34 bar in, 4 bar out, 241 to 144 degrees C

Two phase flow at the throat, and that is where the seat dies

Spent liquor to evaporation

clear liquor, 180 to 200 g/L Na2O

100 to 130 degrees C, 2 to 4 bar

Scale, and caustic cracking where the insulation stops

Red mud washing and disposal

35 to 50 percent solids, pH 12 to 13

60 to 90 degrees C, 1 to 3 bar

Wear on the ball, and settlement in every dead volume

Read the fifth row twice, because it is the only row in the table where a valve is asked to remove thirty bar in one step, and it is also the row that gets specified by copying the row above it. A blowdown valve is bought on line size, flange pattern and body material, which are the three things that matter least.

2. Two duties that should never share one body

Isolation wants a full bore, a seat that seals dead tight, and a flow path with nothing in it to wear. Letdown wants a restricted passage, an expanded outlet, a hardened surface where the energy is dissipated, and above all a velocity ceiling. These are opposing requirements and a ball valve is unusually bad at satisfying both, because its bore is the largest in the plant when open and its seat gap is among the smallest when closed.

Take a 300 cubic metre per hour blowdown line in DN200. The bore area is 0.0314 square metres, so the pipe velocity is 2.65 metres per second, which is exactly where a 35 percent solids slurry should be run and is the reason the pipe lasts fifteen years. Now close the valve to the point where the flow passes a gap whose area is four percent of the bore. The same mass now crosses 0.00126 square metres at 66 metres per second. Nothing about the fluid changed. The valve did that.

At twenty five times the pipe velocity, each particle carries 625 times the kinetic energy, and erosive metal loss climbs steeply with speed, somewhere between the second and the third power of it depending on whether impact or cutting dominates. That is a factor of three thousand at one end and fifteen thousand at the other. This is why a blowdown trim can disappear in nine weeks in a line whose pipe has a fifteen year life, and why the maintenance department, looking at a pipe that is fine and a seat that is gone, concludes that the seat material must be wrong.

3. Thirty four bar to four, in ninety volumes

The blowdown is not a pressure drop in the ordinary sense. It is a flash. Saturated water at 34 bar absolute is at 241 degrees C with an enthalpy of 1037 kilojoules per kilogram. At 4 bar absolute the saturated liquid enthalpy is 604.7 and the latent heat is 2133.8. The fraction that has to boil to get from one state to the other is (1037 minus 604.7) divided by 2133.8, which is 0.20. One fifth of the water turns to steam in the time it takes to cross the seat, and it does so by taking heat out of the remaining four fifths, which is why the downstream temperature is 144 degrees C and not 241.

Now the volume. A kilogram of slurry at 35 percent solids, with solids at 3000 kilograms per cubic metre and liquor at 1150, occupies 0.00068 cubic metres. After the flash, 0.132 kilograms of steam at 0.4624 cubic metres per kilogram takes 0.061 cubic metres on its own, and with the residual liquor and the unchanged solids the mixture occupies 0.0616. The fluid has expanded ninety times, in a distance of a few millimetres, at the one place in the valve where the passage is narrowest.

That is the whole mechanism, and it has a practical consequence that is easy to state and hard to enforce: a ball valve can isolate this line, and it cannot let it down. If a ball valve must be used for letdown, three things have to be true. The pressure has to be broken at the outlet rather than at the seat, which means a cage or an angle body rather than a plain ball. The trim has to be tungsten carbide rather than hardfaced, because quartz is harder than Stellite. And the valve must never be operated below about 30 percent open, because below that the same flow passes a smaller gap at a higher velocity, and the wear rate rises faster than the flow falls.

4. The groove cannot be reached, and that is the point

Look again at where the wear is. It is not on the ball generally and not in the bore. It is an annulus exactly at the seat contact line, because that is the one place where the gap is at its minimum and the velocity at its maximum. Once a groove of 0.2 millimetres exists, the gap has widened by 0.2 millimetres, the leakage has risen roughly in proportion to the cube of the gap, more liquor flashes, the local velocity goes up, and the groove deepens faster. The wear is not a linear process with a rate. It is a feedback loop with a threshold.

The second half of the trap is geometric. A seat in a soft seated valve has 0.3 to 0.5 millimetres of compression available and a metal seat has perhaps 0.1 millimetres of elastic travel. A groove four millimetres deep is eight to forty times beyond anything the seat can follow. The valve does not leak because the seat is worn out in the sense of having lost its spring. It leaks because the sealing line has moved into a trench that the seat cannot enter.

And the wear does not spread out. A quarter turn ball valve has one travel of ninety degrees from stop to stop, so the ball presents the same two bands to the seat every time it closes. There is no indexing, no rotation of the contact patch, no distribution of damage around the sphere. Two bands, machined from both sides, for the whole life of the valve. Any design change that claims to improve slurry life by hardening the ball without addressing the fact that the same band takes every cycle is only moving the failure date.

5. Red mud is harder than the metal, and only one of six components matters

Red mud is not a substance, it is a residue, and its abrasiveness is decided by one minor constituent. The iron reports as hematite and goethite, the titanium as anatase, the silica as a desilication product and, in the fractions that were never dissolved, as quartz. Those five have hardnesses spanning a factor of four, and the metal has a hardness that sits below all of them.

Phase in the slurry, or metal in the valve

Vickers hardness

What it does at the seat line

Gibbsite, the alumina being dissolved

200 to 300

Nothing; it is softer than the seat

Goethite, FeOOH

500 to 600

Polishes the seat face and rounds the contact band

Anatase and rutile, TiO2

600 to 800

Cuts, slowly, and is present in every ore

Hematite, Fe2O3

700 to 900

Cuts; the main abrasive in most red muds

Quartz, SiO2, 0.5 to 3 percent of the ore

1000 to 1100

Cuts tungsten carbide, given velocity and time

316L body, ball and seat carrier

150 to 200

The material being cut, by a factor of four to six

Stellite 6 hardfacing

400 to 450

Survives hematite, loses to quartz at blowdown velocity

Tungsten carbide, 88 percent WC with cobalt binder

1100 to 1400

The only metallic option in the same class as quartz

Two conclusions follow that contradict common purchasing practice. The first is that abrasion resistant stainless steel is a contradiction in terms here: a 316L seat is a quarter as hard as the hematite in the fluid it is sealing against, and no amount of chromium changes that. The second is that Stellite, the default answer for slurry trim in most of the industry, is still 600 Vickers below quartz; it works in coal and it works in ash, and it fails in a diaspore red mud that carries free silica.

Trim material

Velocity ceiling at 35 percent solids (m/s)

Why the ceiling is there

Carbon steel body, uncoated

2 to 3

Uniform metal loss becomes visible wall thinning within a year

316L, uncoated

3 to 4

Better corrosion, no better hardness; the limit is mechanical

Duplex 2205

4 to 5

Higher strength, marginally higher hardness, same wear family

Stellite 6 overlay

5 to 7

Survives hematite, is cut by quartz above this

Tungsten carbide coating, HVOF, 150 to 300 micrometre

6 to 9

Hard phase equals quartz; life set by the cobalt binder and the coating bond

Solid tungsten carbide insert

8 to 12

No binder path to the substrate; brittle under thermal shock

These ceilings assume a median particle near 100 micrometres and a loading at the high end of normal. They fall when the particles get coarser and they rise, surprisingly, when the loading goes up further, because a dense slurry cushions its own impacts and the particles begin hitting each other rather than the wall. A plant that thickens its feed to debottleneck the clarifier therefore does not see the wear double, and a plant that dilutes to improve settling does not see it halve. Wear is not proportional to tonnes.

6. Caustic does not eat the body, it cracks it

The general corrosion rate of carbon steel in Bayer process liquor is low, of the order of 0.05 to 0.2 millimetres a year, because the caustic passivates iron as magnetite and the liquor is essentially free of oxygen. A 25 millimetre body wall losing a tenth of a millimetre a year is not a problem, and that is the reason carbon steel is the right choice for digestion vessels, flash tanks and most of the piping in a refinery. Reading only the corrosion rate, a carbon steel valve body looks safe for a century.

Caustic stress corrosion cracking is a different failure and it does not appear in a corrosion rate. Carbon steel cracks intergranularly in sodium hydroxide above roughly 5 to 10 percent concentration and above 50 to 60 degrees C, provided there is tensile stress at the surface and the caustic is concentrated at that surface. Spent liquor at 200 grams per litre of sodium oxide is about 20 percent sodium hydroxide by weight, and the digestion train runs at 145 to 260 degrees C. Every wetted carbon steel surface in the train is inside the cracking window; the only variables are stress and concentration.

Concentration is the one that catches people out, because it happens in places nobody instruments. A flange that weeps, an insulated body whose lagging has been wetted and dried a hundred times, a gland area where liquor evaporates between strokes, all concentrate sodium hydroxide towards 50 percent and above, and all raise the cracking susceptibility by an order of magnitude without raising the bulk concentration at all. This is the same mechanism that cracked riveted boiler seams in the nineteenth century, and the countermeasure has not changed: remove the stress rather than the caustic.

In practice that means post weld heat treatment of the body at 620 to 650 degrees C after every weld, including repairs done in the field, with a furnace chart in the documentation package rather than a certificate that says stress relieved. It means no cold formed bends, no welds ground flush and left in tension, and no hard stamping on a pressure boundary. It also means that duplex is not the answer: the ferrite phase is selectively attacked in hot concentrated caustic, and 2205 at 200 degrees C in 20 percent sodium hydroxide is a worse choice than stress relieved carbon steel. Where the concentration and temperature both go up, the reference material is nickel 200, at the cost of half the strength and all of the price advantage.

7. Scale grows where the heat is, and the seat is the hottest cold spot

The liquor leaving digestion is supersaturated in silica and in sodium aluminate, and it deposits a desilication product, a sodalite family scale, on hot surfaces at rates from 0.1 to 1 millimetre a month depending on the silica load and the temperature. The scale is not removed by acid, only by hot caustic wash or by mechanical means, and its thermal conductivity is around 1.5 watts per metre kelvin against 45 for steel, so a two millimetre layer behaves like thirty millimetres of wall as far as heat transfer is concerned.

That matters to a valve for one reason. Scale does not grow evenly, and it does not grow at all on a surface that is being wiped. The ball wipes a band twice per cycle. The seat ring face and the cavity behind it do not get wiped, so the scale builds preferentially on the stationary part, the seat contact becomes a scale on metal contact rather than metal on metal, and the valve begins to leak at a few tenths of a millimetre of lift. From there the mechanism is the one described earlier: leak, flash, velocity, groove. Scale is not a fouling nuisance that reduces Cv. In this service it is the trigger for the wear that everyone then blames on the abrasive.

8. Six clauses that would have doubled the life of that valve

  1. Name the duty, and allow only one. Isolation or letdown, in the datasheet, with a line that says the valve will not be used for the other. Every blowdown valve in a refinery has been used for both.

  2. Set the velocity ceiling at the worst case, not the nominal. The number that governs is at minimum controllable flow and maximum solids, in metres per second at the seat gap, not cubic metres per hour on the line.

  3. Specify hardness in Vickers with the phase named. Tungsten carbide 1100 to 1400 HV with the binder percentage stated, or Stellite 6 at 400 to 450 HV with an acceptance that it will not survive free quartz. A drawing that says hardfaced is a drawing that says nothing.

  4. Require a flush connection at the lowest point of the cavity, one inch minimum, with the flush pressure and the flow rate stated, and a note that the connection must be rodded out at every shutdown because a 60 percent solids sediment will plug it in one outage.

  5. Require post weld heat treatment after all welding, at 620 to 650 degrees C, with the chart, and a hardness survey of the heat affected zone on the certificate.

  6. Quote torque at the end of the specified interval, with the deposit allowance named. A DN200 class 300 valve that turns on 1500 newton metres when clean will demand 4500 to 7000 with a scaled seat and a settled cavity, and an actuator sized on the clean figure will stall in the second year and be diagnosed as an instrument fault.

9. Where J-VALVES fits

The arguments in this article are all settled on paper, and the paper needs three numbers on it: the differential, the temperature and the solids. J-VALVES builds the bodies, balls and seat carriers that those three numbers describe, and issues the torque curve measured at the differential the order names rather than a single figure taken in air at ambient. The catalogue covers bores from DN15 to DN1400, a half inch to 56 inches, in ASME classes 150 through 2500, across 846 kelvin of temperature from 196 below zero to 650 above it. Shells are taken to 150 percent of rating before dispatch and seats to 110 percent, and the two certificates are separate documents, each recording the side the pressure was applied from. An enquiry that states the differential, the solids loading and the seat material comes back as a priced drawing inside three working hours, and it will say which of the six clauses above the standard design already meets.

10. The one line to remember

A ball valve in a Bayer plant is not eaten by the caustic and it is not worn out by the mud. It is machined by its own seat clearance, at a velocity created by a flash that only happens because the valve is nearly closed, and it does that to itself on the same two bands of the same ball for as long as it is in service.

11. Frequently Asked Questions

Can a 316L ball valve be used on red mud service?

It can be installed and it will not corrode quickly, because the liquor passivates stainless steel and the corrosion rate is low. It will wear out, because 316L runs at 150 to 200 Vickers and the hematite in the mud is 700 to 900 and the quartz is 1000 to 1100. A 316L seat is being cut by an abrasive four to six times harder than itself, so the only question is how many weeks it lasts. If the line is an isolation valve at 2 metres per second it may last years; if it is a blowdown at 66 metres per second at the seat gap it will not last a quarter.

What velocity should a red mud slurry be limited to through a ball valve?

Between 2 and 3 metres per second for carbon steel, 3 to 4 for 316L, 5 to 7 with Stellite hardfacing and 6 to 9 with tungsten carbide, at a median particle near 100 micrometres and 35 percent solids. Those figures apply to the velocity at the narrowest passage, which in a ball valve is the seat gap and not the bore. A DN200 line running 300 cubic metres per hour has a bore velocity of 2.65 metres per second and a seat gap velocity above 60, and it is the second number that sets the life.

Why is caustic stress corrosion cracking more important than corrosion in a Bayer plant?

Because the uniform corrosion rate is negligible and the cracking is not. Carbon steel loses 0.05 to 0.2 millimetres a year in Bayer liquor, which is a century of life on a 25 millimetre wall, but it cracks intergranularly in sodium hydroxide above about 5 to 10 percent and above 50 to 60 degrees C when there is tensile stress. Spent liquor at 200 grams per litre of sodium oxide is roughly 20 percent sodium hydroxide, so the whole train is inside the window and the only defence is post weld heat treatment at 620 to 650 degrees C and the avoidance of concentrated caustic at wetted insulation and weeping flanges.

Should the digestion blowdown be a ball valve at all?

Not for continuous letdown. A 34 bar to 4 bar flash expands the fluid about ninety times at the seat, drives the throat velocity to 60 metres per second and above, and puts the entire pressure drop across the one surface that must also seal. A cage trim, an angle body or a dedicated letdown device with an expanded outlet will last longer for the same alloy. A ball valve is the right choice upstream and downstream of that device, where the job is isolation and the velocity is the pipe velocity.

What seat leakage class is achievable with a metal seat in this service?

ISO 5208 rate D, and it should be written into the specification as rate D with the test fluid named, because rate A on a bench with clean water is achievable and rate A in service is not. The reason is arithmetic rather than workmanship: a metal seat has about 0.1 millimetres of elastic travel, and the first groove that forms at the contact band is deeper than that within weeks. A specification that asks for rate A and receives a certificate for rate A has bought a bench result, and the first month of operation will convert it into a rate D valve with a groove in it.

Related Products

Explore the Valves in This Article
Nominal Size: 1 inch / DN25, range 1/4 to 12 inch Pressure Class: ASME Class 150, 19.6 bar at 38°C; Class 300 optional Body Material: ASTM B148 C95800 nickel aluminum bronze Body Type: Two piece, bolted Ball: C95800, SS316 hard faced optional Stem: C95800 or SS316, blowout proof Seat: PTFE, RPTFE, PPL, or reinforced PTFE Packing: PTFE or graphite combined packing End Connection: Threaded NPT / BSPT, flanged RF to ASME B16.5 optional Service Temperature: -29°C to +150°C standard, +200°C high temperature version Seawater Velocity Limit: About 6 m/s clean, 4.5 m/s with sand Design Standard: API 608, ASME B16.34 Test Standard: API 598, ISO 5208 Operation: Lever standard, pneumatic or electric optional
Size Range: 2 to 56 inch (DN50 to DN1400) Pressure Class: ASME Class 150 to 2500 / PN20 to PN420 Body Material: WCB, LCB, CF8, CF8M, CF3M, duplex, alloy steel Ball: Stainless with hard chrome, ENP, Stellite or tungsten carbide overlay Seat: PTFE, RPTFE, PPL, or metal Stellite faced Seat Arrangement: SPE, DPE (DIB-1), or combination (DIB-2) Packing: Live loaded graphite, ISO 15848-1 qualified Fire Test: API 607, also API 6FA and ISO 10497 Fugitive Emission: ISO 15848-1 class B or A, with temperature and cycle class stated Face to Face: ASME B16.10 short or long pattern End Connection: Flanged RF / RTJ to B16.5 and B16.47, butt weld to B16.25 Features: Double block and bleed, sealant injection, anti-static, anti-blowout stem Design Standard: API 6D, API 608, ASME B16.34, ISO 14313 Operation: Lever, gear, pneumatic, electric, hydraulic, gas over oil Sour Service: NACE MR0175 available
Nominal Size: 1-1/2 inch / DN40 Pressure Rating: 1000 WOG (68.9 bar cold working, non-shock) Body Type: Three piece, bolted end caps, four body bolts Body Material: ASTM A351 CF8 (304), CF8M (316) optional Ball: CF8, polished Ra 0.4 µm, full or reduced bore Seat: PTFE, RPTFE, PPL, or Stellite faced metal Body Gasket: PTFE to 180°C, graphite above Packing: PTFE V-ring to 200°C, graphite above End Connection: NPT, BSP, socket weld B16.11, butt weld B16.25, flanged RF Actuator Mounting: ISO 5211 F05 / F07 pad Air Supply: 0.4 to 0.7 MPa clean dry air Service Temperature: -29°C to +260°C, seat dependent Design Reference: MSS SP-110 general purpose, ASME B16.34 body wall Test Standard: API 598, ISO 5208
Nominal Size: 3/4 x 1/2 inch (DN20 x DN15), reduced bore Pressure Class: ASME Class 600 / PN100, 102.1 bar at 38°C Body Material: ASTM A182 F51 forged duplex, UNS S31803 PREN: Approximately 35 Ball: F51 with HVOF tungsten carbide or Stellite overlay Stem: F51, SS316 or 17-4PH, blowout proof Seat: RPTFE, Devlon, PEEK, or Stellite faced metal Bolting: B8M Class 2, alloy 718, or B7M for sour service End Connection: NPT, BSP, socket weld ASME B16.11, butt weld ASME B16.25 Bleed Port: Cavity bleed with plug or needle valve, lockable option Service Temperature: -29°C to +300°C, seat dependent Design Standard: API 6D, API 608, ASME B16.34 Test Standard: API 598, ISO 5208, cavity test through bleed port Sour Service: NACE MR0175 available